Showing posts with label CARDING. Show all posts
Showing posts with label CARDING. Show all posts

Flat card and cotton drawing frames

This machine is intended to clean and parallelise the fibres and to produce a card sliver in which fibres are regularly distributed (Fig. 4).

The card carries out also a cleaning action. The careful study of the clothings and of the air passages permitted to increase further the productivity of these machines.

clip_image0443

An industrial production of 50-60 kg/h has become to-day a quite usual reference. This result has been attained by further developing following features:

· the feeding of a batting of constant count, well opened and sufficiently cleaned

· a more intensive opening and cleaning action, by the licker-in, with an effective waste removal

· the improvement of the suction system

· the automatic control of the sliver regularity and quality, in terms of neps.

The cotton drawing frames

The purpose of this machine is to parallelise the fibres by doubling and drawing several slivers.

In order to produce a sliver with maximum regularity, automatic adjustment systems are used for reducing short-, medium- and long-term variations in the sliver weight. In fact sensors are used to measure the variations in sliver weight, and the consequent necessary corrections are applied by varying the draft, that is the speed of the delivery rollers as compared to the feed rollers.

Depending on the envisaged end-product, one or two drawing frame passages can be made. This processing stage is extremely important for the regularity of the end-product, as the following machines (the roving frame and the spinning frame, both ring and rotor frame) cannot correct any more the weight irregularities of the roving and of the yarn.

Read more...

Carding And Spinning system–Improvement & Research

DYNAMIC ANALYSIS AND DEVELOPMENT OF CARD-SPINNING SYSTEM
PROJECT GOAL
The goal of this project is to create the fundamental knowledge needed to develop more efficient machines and novel processes that can potentially decrease the number of process steps by a factor of 2 to 3 in short staple yarn manufacturing.
ABSTRACT
To develop more efficient machines for short staple yarn manufacturing that can significantly shorten the processing line, we are currently conducting research in the following two interrelated areas: (1) to analyze the motion dynamics of fiber clumps and particles in an airflow field, and (2) to develop a single-step process (Card-Spinning) to incorporate multiple spinning heads into a carding unit. This involves a fundamental analysis and understanding of web uniformity monitoring, measurement, and regulation, web division, and feeding of web ribbons into yarn spinning heads positioned at the front end of the card.
We have built a prototype of the yarn spinning head system and have modified opening and carding machines to demonstrate the concept. A series of yarns has been made with the spinning head system by varying the process settings. Evaluation of these yarns indicates that the technology is promising and further development is underway.
We have frequently interacted with our industrial partners including yarn producers and machinery manufacturers to share information on the project and to learn the state of the art practice in the industry. Studies are underway on theoretical and experimental analysis of airflow, and on the development of the Card-Spinning system.

INTRODUCTION
In the past decades, yarn manufacturing has transformed from a labor intensive operation to a capital intensive one. This change has allowed the US to remain competitive in the global marketplace. Although the productivity of current manufacturing systems continues to increase,
a significant improvement requires major breakthroughs and new innovations, which can only be achieved with a better understanding of the fundamental principles of the processes.
Staple yarn manufacturing involves four essential operations: fiber separation, parallelization, attenuation, and consolidation. Currently, several machines (about 10) in sequence are needed for these tasks. We are developing the fundamental knowledge base that can lead to more efficient machines, shorter production lines, and novel processes. Our first major task in this project is the study of the motion dynamics of fiber clumps and particles in an airflow field. The second major task aims at developing a novel process (Card-Spinning) by incorporating multiple spinning heads on the carding machine itself.
AIRFLOW IN OPENING AND CLEANING
The opening and cleaning process is the first part in a staple yarn manufacturing line. It opens fiber bales into small tufts, removes most of the impurities, and blends fibers together. Airflow plays a very important role in determining the efficiency and quality of the opening/cleaning operations. Fiber opening, cleaning, and transport in the opening and cleaning processes are achieved through interactions among airflow, inertia forces, gravity, fiber/particle configurations, barrier arrangements (mote knives, grid bars, plates, etc.), beating actions, carding actions, among others. Although some studies have been conducted in this area (e.g., [1] on opening and cleaning and [2,3,4] on carding), the depth has been limited due to the complexity of the problem.
The airflow with particles and fibers in these processes is typically a two-phase, unsteady viscous flow. Our studies include experimental analysis using flow visualization techniques and computational fluid dynamics (CFD) analysis. The experiments were designed to determine the effect of fibers on airflow pattern, and to determine the condition when fibers can be neglected in a CFD analysis. Some of the test results have been used to build a two-phase flow model in CFD. One of the uses for the model is for predicting the flow characteristics and improving the design of textile machinery.
Test setup and pressure distribution
The test setup, shown in Figure 1, is designed so that the test section can be changed to obtain typical flow patterns such as parallel, diverging, converging and flow over a bent section. It is an enclosed system consisting of a fan, test section and connection pipes. The test section is a rectangular channel (1.5 m X 0.15m X 0.31m), the top of which can be adjusted or replaced to change the shape of the channel. It is built with plexiglass panels to enable flow visualization using a high-speed video camera. Forty pressure sensors arranged in four rows are installed to monitor the flow pattern.
clip_image002
The pressure in the test section was measured with the flow channel in the expansion type flow configuration. With this configuration, a pressure increase should be seen along the flow direction. The experimental results were compared to those of the CFD model (Figure 2). The trends seen in the experimental results agreed well with those of the model, however, a difference in the magnitude of the pressures was seen. The difference in magnitude was not of concern, since a more meaningful comparison is done by looking at the slopes of the experimental and model results. This comparison shows good agreement between the CFD model and the experimental observations. Upon further investigation, a temperature increase was observed in the test system. This causes a reduction in the density of air, which changes flow rate. When the influence of this temperature increase is included in the modeling, the results are only 12% different than the experimentally observed data.
Influence of amount of fiber in the flow and velocity of fibers in air flow
A series of tests were conducted to determine the sensitivity of the flow field to increases in the amount of fiber present. The amount of fiber in the test setup was changed (approximately 35 g, 69 g, 98 g,119g and 141 g) for each series of experiments. To determine the velocity of fibers in the airflow in the test section, a high-speed video camera is used to capture images of airflow with a foam particle which is similar in dimensions to the fiber clumps. Results showed that the velocity of the foam particle ranged from 7.52 to 16.8 m/sec with an average of 12.6 m/sec. The average velocity of the air flow in the test setup without the particle was 11 m/sec. These results have been analyzed and found to be reasonable.
In summary, we have built a test setup that captures many of the characteristics of flow fields present in textile machinery. We have demonstrated that CFD models can be used to predict the trends seen in the pressure distribution for the test setup for both air and air-fiber flow. The trends in the experimental data for varying amounts of fiber in the flow were captured by the model. However, the models do not predict the exact values of the pressures. Further
development of the models will lead to better predictions of the experimental data. In the future, the results of the models will be used to design new textile processing equipment.
CARDING
In a traditional process, carding individualizes fibers, removes fine impurities and neps, and forms a sliver. By incorporating multiple spinning heads on the carding machine itself, the novel Card-Spinning machine will replace the traditional card, two draw frames and the yarn-spinning machine.
Web monitoring
One of the major problems in spinning multiple yarns directly from a card web is that the cross-machine web density must be monitored and the divided sections must be controlled. Although some studies on web uniformity have been conducted for nonwoven processes [5,6,7,8,9], there is no available data on cross-machine uniformity for the card in yarn production line since the web is typically condensed into a single sliver and only the overall linear density is important. When one decides to split the web into multiple sections to feed directly to spinning heads, the variability of the web takes on great importance.
A system has been integrated with the card to monitor the web density on-line. It employs a computer, line-scan camera and high-speed frame grabber board (Figure 3). This system will enable real-time monitoring across the full width of the web. This is important for monitoring the input quality of the web to the yarn-spinning head. The system is capable of monitoring 100% of the web or just sampling a subset of the web. An image of the web is created line-by­line with the scanning rate of the camera synchronized with the web motion when 100% monitoring is required. In this way a picture of the web is obtained. For process monitoring and control, a statistical sampling can be taken to analyze variation in any given section (strip) of web. An extensive literature search did not find published data on web variability and this work should add to the body of knowledge.
Web splitting
A proof-of-concept device has been designed and the first prototype was built. The principles involve positive control of the web sections during division via belts that squeeze the web, and through differential speeds, shear the web longitudinally in a short distance. Servomotors with digital control were added to the device (Figure 4). Initially, the belts were divided into two groups with slower and faster speeds, each set driven by one servomotor. It was found that the slower motor’s speed was influenced due to frictional drags caused by the adjacent faster moving pulleys. The device was then modified to use timing pulleys and belts to ensure an accurate speed difference. Effort to synchronize the speeds of the web divider, card, and yarn spinning heads is underway. When the concept is finalized, the apparatus can be easily expanded to 10 or more strips. The limitation, of course, is in the uniformity of the web across the
clip_image004
machine. It is expected that uniformity of polyester staple fibers will produce a reasonably uniform web. A cotton web would be much more of a challenge. The web will be made as heavy as possible in order to create the linear density needed for a coarse yarn.
YARN FORMATION BY CARD-SPINNING
In a traditional staple yarn spinning system, fibers are opened, cleaned, carded, drawn and reduced to a roving before spinning (twisting). One of the objectives of this project is to design a system where the short staple fibers in the carded web can be spun directly into a yarn before the web is consolidated into a sliver. A literature research (e.g., [10,11,12,13]) shows that efforts have been made to shorten the systems to convert short staple (cotton type) fibers into yarns, and that in the shortened systems, carded or drawn sliver is processed into either a ring spun, a rotor spun or an air jet spun yarn, thus eliminating the extra step of drawing and/or roving.
We have assembled a flexible "hybrid nozzle" spinning device with the objective of straightening the fibers, twisting the bundle with high efficiency and low air consumption, and producing a smooth and strong yarn. Figure 5 shows a schematic drawing of the spinning device, and Figure 6 shows a photograph of the device. The device is designed to have the maximum flexibility in processing conditions. It is placed on a height-adjustable table with wheels. The speeds of the feeding rollers, delivery rollers and the winder can be independently set.
In conventional airjet spinning machines, a draft system is used to draft and to feed the fiber strand into the spinning nozzle. For example, MJS801 air-vortex spinning machine by Murata has 3-roll drafting system while MJS802 has a 4-roll system. In our Card-Spinning system, because the card web is split to provide the necessary linear density, there is no need to draft the web ribbon. Therefore, a pair of normal feeding rollers are used to control the rate of feeding the web ribbon into the spinning nozzle. The vortex air spinning unit is composed of a Murata 802 MJS, twin air jet spinning nozzle, and utilizes a service air system. A negative air pressure is formed in the first nozzle to aspirate the fiber sliver. The second nozzle twists the outer fibers free from fiber core to wrap around the core and form a yarn. A pair of delivery rollers and a winder is used to wind the yarn into a cone shape that is suitable for further experimental tests and production.
Before this spinning device is directly attached to the web splitting device under development (see previous section), we tested its operation by feeding it with separately prepared thin slivers. The feed strand is aspirated into the spinning unit via a transfer channel. The fiber bundle is twisted to form a yarn, which is then wound onto a paper cone.
In a conventional airjet spinning process, drawn slivers are used as the feeding stock. Whereas for the Card-Spinning device, card web will be fed to the spinning device directly. To study the effect of feed stock, we have conducted a study to compare the yarn characteristics using both drawn sliver and card sliver as the feed material. The feed slivers, of the same linear density, were fed into our spinning device to produce yarns under the same spinning parameters: air-
clip_image006
pressure of spinning nozzles, feed speeds, delivery speeds and windup speeds. The analysis on the final yarns shows that yarns spun from card sliver are not as uniform as that of yarns from drawn sliver. However, the card sliver, due to its loose structure, is easier to twist.
The main factors influencing the final yarn qualities include: super feeding ratio (affecting winding tension); condenser size; distance from front roll to spinning nozzle and air pressures. Three air-pressure conditions and two super feeding ratios were used to produce yarns with drawn sliver and card sliver (Table 1). The effect of feed ratio, pressure ratio, and feeding stock on yarn breaking strength is shown in Figure 7.
For the carded sliver yarns, a nozzle pressure ratio of 0.57 yielded a yarn with better final yarn quality than the yarn produced with other ratios. For example, the tensile strength of yarns with
clip_image008
P= 0.57 ranged from 1.6 to 2.0 kgf, while those produced with P = 1.78 and P = 3.0 were significantly weaker (0 to 0.5 kgf). Yarn elongation and tenacity exhibited a similar trend.
For the drawn sliver yarns, a value of P=1.78 yielded the highest tenacity and elongation. A feed ratio of 0.98 was shown to produce the highest quality yarns.
In analyzing the effects of drawing on yarn characteristics, it was shown that for P ratios of 1.78 and 3.0, the drawn sliver produces a better quality of yarn. However, for P = 0.57, the carded sliver yields better yarn quality. This was determined by evaluating the yarn strength, yarn elongation and yarn tenacity. This result is significant. It means that if the fiber alignment and desired regularity of a sliver are achieved by carding machine modification, the spinning of yarn directly from carded web may be practical. The expensive drawing process could then be eliminated from the staple yarn production line. Further details are presented in the thesis derived from this systematic study of processing parameters [14].
SUMMARY
This project focused on the motion dynamics of fiber clumps in an airflow field and the development of a prototype Card-Spinning unit, which combines carding and yarn spinning in a single machine. We have demonstrated its feasibility in producing coarse yarns. Continuing effort is underway on experimental and theoretical analysis of air flow, web uniformity regulation, system integration/enhancement, and yarn characteristics studies.
We are pleased that the project has received significant interest and support from the textile and the machinery industries. The interaction with industrial partners plays a significant role in the success of this project.
clip_image010
Investigators: Youjiang Wang (leader), Mary Lynn Realff, Radhakrishnaiah Parachuru, J.
Lewis Dorrity, Fred L. Cook, Jim Brazell, Xi Chen (Georgia Tech)
Bhuvenesh C. Goswami, David A. Zumbrunnen (Clemson)
Students: Shumin Zheng, Fan Zhao, Hua Huang (Georgia Tech)
Kai Liu, John Mike Wolf (Clemson)
Read more...

CARDING (textile) Process parameters

INTRODUCTION:
Carding is the most important process in spinning. It contributes a lot to the yarn quality. The following process parameters and specifications are to be selected properly to produce a good quality yarn with a lower manufacturing cost.
cylinder wire(wire angle, height, thickness and population) flat tops specification licker-in wire specification doffer wire specification feed weight draft between feed roller and doffer cylinder grinding doffer grinding flat tops grinding cylinder, flat tops, doffer wire life Licker-in wire life Cylinder speed flat speed Licker-in speed setting between cylinder and flat tops setting between licker-in and feed plate setting between licker­in and under casing elements like, mote knife, combing segment etc. setting between cylinder and doffer setting between cylinder and back stationary flats setting between cylinder and front stationary flats setting between cylinder and cylinder under casing
CYLINDER WIRE AND CYLINDER SPEED
Cylinder wire selection is very important, it depends upon cylinder speed, the raw material
to be processed and the production rate. The following characteristics of cylinder wire should be considered.
1. wire angle
2. tooth depth
3. wire population
4. rib thickness
5. tooth profile
6. tooth pitch
7. tooth point
8. overall wire height
Wire front angle depends on mainly cylinder speed and coefficient of friction of raw material.
Higher the cylinder speed, lower the angle for a given fibre. The cylinder speed in turn depends upon the production rate.
Higher production means more working space for the fibre is required. It is the wire that keeps the fibre under its influence during carding operation. Therefore the space within the wire should also be more for higher production. Higher cylinder speed also increases the space for the fibre. Therefore higher cylinder speed is required for higher production.
In the case of high production carding machines, the cylinder surface is very much higher, therefore even with higher number of fibres fed to the cylinder, the cylinder is renewing the carding surface at a faster rate.
Higher the cylinder speed, higher the centrifugal force created by the cylinder, this tries to eject
the fibre from the cylinder, along with the trash. It is the cylinder wire's front angle which overcomes the effect of this force. Low front angle with too low cylinder speed and with high frictional force will result in bad quality, because the fibre transfers from cylinder to doffer will be less. Hence recycling of fibres will take place, which result in more neps and entanglements.
The new profile with less free blade avoids loading of the cylinder with fibre and/or trash.
This helps in keeping the fibres at the tip of the tooth. The movement of the fibres towards the
tip of the tooth coupled with centrifugal action demands an acute front angle to hold the fibre in place during carding.
Lack of stiffness associated with fine and/or long fibres necessitates more control during the carding process. This control is obtained by selecting the tooth pitch, which gives the correct ratio of the number of teeth to the fibre length. Tooth pitch reduction is therefore required for exceptionally short fibres and those lack stiffness.
Number of points across the carding machine is decided by the rib width. It is selected based on the production rate and fibre dimensions. Finer the fibre, finer the rib width. The trend is to finer rib width for higher production.
The population of a wire is the product of the rib thickness and tooth pitch. The general rule is higher populations for higher production rates, but it depends upon the application.
Sharp tooth points penetrate the fibre more easily and help to intensify the carding action. Cut-to-point wires are sharp and they have no land at all.
The effective working depth of a cylinder wire tooth for cotton is approximately 0.2mm and for synthetic materials approx.0.4mm. Manmade fibres require more space in their cylinder wire than doe's cotton. More tooth depth allows the fibre to recycled, resulting in damaged fibres and neps. If tooth depth is insufficient, there will be loss of fibre control. This will result in even greater nep generation. Looking into the above details, the following specifications can be used as a guideline

clip_image002
clip_image004
DOFFER, LICKER-IN AND FLAT TOPS:
· The basic function of doffer is to strip the fibres from Cylinder. Please remember that the action between cylinder and doffer is carding action (or combing action or point to point action).
· The doffer wire's front angle plays a very important role in releasing the fibre from the cylinder. For most carding applications the optimum angle is 60 degrees.
· Increased population over 400 ppsi does not give any advantage in the production of quality yarn. For smaller doffers, 5 mm doffer wire height helps in transferring the fibres from cylinder to doffer.
· If the fibre holding capacity of the doffer wire is less due to fibre friction or due to very high doffer speed, it is better to use a doffer wire with striations. For high production carding itis always better to use doffer wire with striations.
· Licker-in plays a major role in opening the fibre tufts. In general 85 degrees is used both for synthetic and medium and long cottons. For coarse and dirty cottons 80 degrees can be used.
· Strength, hardness and sharpness are very important for Lickerin wire. Licker-in wires should never be ground. Thinner blades penetrate the fibres more efficiently and increase the wire life.
· Higher number of rows per inch gives better results. Now up to 12 rows per inch is being used. This is always better compared to 8 rows per inch.
· If the wire pitch is not sufficient, it can be compensated by increasing the licker-in speed. Higher licker-in speeds for fine and long cottons will rupture the fibres. Licker-in speed depends upon the fibre type and the production rate.
· It is better to use a flat top with more than one population. The general combination is 280/450. This is suitable for both cotton and synthetics. Please remember that the rigidity of the fillets is different for cotton and synthetic. If cotton flat tops are used for synthetic processing, the load on the cylinder will be more, more heat will be produced and hence the probability of cylinder loading due to electrostatic charge will be high.
· Instead of using Rigid type flat tops, it is better to use semirigid type flat tops while processing synthetic fibres.
SETTINGS:
· The setting between cylinder and doffer is the closest setting in the card. This setting mainly depends upon the cylinder speed, hank of the delivered sliver and the type of wire. Cylinder speed up to 360, the setting should be 0.1mm. For cylinder speeds more than 450, the setting ranges from 0.125 to 0.15.
· If the setting between cylinder and doffer is very close, the wires will get polished and this will affect the fibre transfer. If the setting is too wide, the fibres will not be transferred to doffer from the cylinder, hence cylinder will get loaded. While processing synthetic fibres cylinder loading will badly affect the yarn quality. Moreover, it is difficult to improve the wire condition if the loading is severe. The only solution would be to change the wire. Therefore enough care should be taken while processing synthetic fibres.


· The most critical setting in a carding machine is between cylinder and flat tops. While processing cotton, it can be as close as 0.175 mm provided the mechanical accuracy of flat tops is good. Since
most of the cards are with stationary flats at the licker-in side, the setting from the back to front for flats can be 0.25, 0.2.0.2, 0.2, 0.2mm.
· Closer the setting between cylinder and flats, better the yarn quality. Neps are directly affected by this setting. Of course, very close setting increase the flat waste. For processing cotton the setting can be 0.25, 0.2, 0.2, 0.2, 0.2mm. For synthetic fibres it can be 0.3, 0.25, 0.25, 0.25, 0.25mm
· Most of the cards are with 6 to 1 1 stationary flats at the licker-in side. This setting can start with 0.4 mm and end with 0.25mm.
· The wire points can start with 140 ppsi and end with 320 ppsi. The work done by the first few stationary flats is very high; therefore the wear of these flats is also high. It would be better if the first 50% of the flats are changed after 100000 kgs of production and the rest after 150000 kgs of production.
· These stationary flats open the material so that, the setting between cylinder and flats can be as close as possible.
· The setting between feed plate and Licker-in depends upon the type of feed plate. Conventional feed plate setting is decided mainly by the feed weight and to some extent by the fibre length and type. With the latest feed plate and feed roller arrangements, the setting is decided mainly by the fibre length and to some extent by the feed weight.
· Normally the setting between the feed plate and Lickr-in is around 0.45 to 0.7mm, depending upon the feed weight and fibre type.
· The setting between Licker-in and the first mote knife is around 0.35 to 0.5 mm. This helps to remove the heavier trash particles and dust. Closer the setting, higher the wastage. The setting between Licker-in and combing segments is around 0.45 to 0.6. This helps to open the material.
· Some cards have two mote knifes in the Licker-in under casing. The setting is around 0.4 to 0.5mm. This helps to remove the smaller trash and dust particles.
· The setting between the cylinder and stationary flats at Doffer side helps to transfer the fibres to doffer by stripping the fibres to the top of the cylinder wire. This setting can be as close as 0.15mm. The number of wire points on stationary flats also plays a major role. It is normally around 300 to 400. For a high production application it can be as high as 600.
· For cotton processing, the stationary flats are fixed with a knife attachment. The setting should be as close as possible, i.e. around 0.15mm. This helps to remove the trash particles of very small size.


· The setting between cylinder and cylinder under casing should be as per the manufacturer's recommendation. The design of under casing is different for different manufacturers. This setting is very important, as wrong settings will affect the fibre transfer and can also create air turbulence.
SPEEDS:
· Higher cylinder speed helps fibre transfer. Higher the production, higher should be the cylinder speed.
· Higher cylinder speed improves carding action, thereby imperfections are reduced.
· Higher Licker-in speed for coarse fibres and dirty cotton helps to remove the trash and improves, br> the yarn quality. For fine and long cottons, higher speed results in fibre rupture, therefore, flat waste and comber noil will be more.
· Higher flat speed, improves yarn quality and at the same time increases the flat waste
· With the same flat speed, higher the carding production, lower the flat waste and vice-versa.
· Very high tension drafts will affect carding U%. It is better to keep the draft between feed rollers to doffer around 75 to 95. The results are found better with these drafts.
WIRE MAINTENANCE:
· For a modern cylinder wire of 2mm height, grinding with the normal grinding stone is not recommended. It is better to use TSG grinder to grind the wire every 2nd or 3rd month, so that the sharpness of the wire is always maintained.
· TSG grinder does not grind the wire, therefore if the wire is worn out very badly the quality improvement using this grinding machine will be nil. Frequent grindings are recommended. If TSG grinder is not available, it is better not to grind 2mm wires.
· The number of traverse should increase depending upon the life of the wire. The number of traverse for successive grindings should be like this 3, 5, 10, 17 etc. Anyway the best method is to confirm with the microscope. If the grinding is not sufficient, the number of traverse should be increased.
· Doffer is still working with a concept of Land formation. A normal grinding machine will be good for doffer grinding. All the wire points should be touched by the grinding stone. A slow and gradual grinding with the grind-out concept will give the best results. Harsh grindings will result in burr formation on the land. This will increase the number of hooks in the fibre; thereby the effective length of the fibre from this card will be reduced.
· Flat tops grinding is very important. Every time a flat top is ground, yarn quality is improved. It is better to use a grinding machine with the emery fillet. Frequent flat tops grinding will result in less neps and the yarn quality will be consistent.
· Some mills increase the life of the flat tops compared to cylinder wire. But it is better to change flat tops and cylinder wire together for better and consistent yarn quality.
· It is a good practice to check the individual card quality before changing the wire.
· Licker-in wire should be changed for every 150000 kgs. Earlier changes will further improve the yarn quality.
· Stationary flats should be changed for every 150000 kgs. But it is a good practice to change the first 3 or 6 stationary flats at Licker-in side for every 100000 kgs. This helps to maximize the carding effect between cylinder and doffer which is critical for better yarn quality.
OTHERS:
· Lower the feed variation, better the carding quality. Even if the card is with an auto leveler, feed variations should be kept as low as possible (plus or minus 10%). With the latest chute feed systems, it is easy to control the feed variation with in 5%. Lower the feed variation, lower the draft deviation, therefore yarn quality will be consistent.
· If the card is with auto-leveller, the nominal draft should be selected properly. Improper selection will affect sliver C.V% and yarn quality.
· Improper feed roller loading and the setting between feed roller and feed plate will affect the quality, especially C.V% and neps.
· Before mounting, the eccentricity of cylinder and doffer should be checked. Eccentric cylinder and doffer will affect the U% and will affect C.V. % also.
· Defective bearings, gears and timing belts will affect U%.
· Uneven distribution of tension drafts will affect U%.
· Selvedge of feeding bat should be good. It should not be folded and double. This will increase the neps and sometimes it may result in cylinder loading. Lap fed to the carding machine should be narrower than the nominal width of the machine.
· For processing cotton, minimum 800 Pascal suction pressures should be maintained at trash master (at knife) for effective removal of trash and dust particles.
· Worn or damaged scraper blades will lead to web sticking to crush rollers. Insufficient pressure between scraper blade and crush roller will also result in web sticking. If the calendar roller pressure is too high web sticking will also be high.
· If Cylinder under casing nose at doffer side is too long for the type of fibre being carded web disappearing problem will arise. If the nose is set too close to the cylinder, web disappearing problem will arise. Damaged and dull doffer wire also will result in web disappearing problem.
To find out more articles please visit www.jayaram.co.nr or mail to manisujai@rediffmail.com
Read more...

Impact of Carding Micro-climate

TEXTILE TECHNOLOGY
The Impact of Carding Micro-climate on Cotton Moisture Content
and Fiber and Yarn Quality

David D. McAlister III*, David T.W. Chun, Gary R. Gamble, Luther C. Godbey,
Dean R. Cobb, and Everett E. Backe
ABSTRACT
Temperature and relative humidity are important considerations for carding cotton in textile manufacturing. It has been suggested that high relative humidity decreases the stiffness of fibers and increases the moisture content of the fibers. With the recent interest in moisture addition at the gin, it is important to determine if increased fiber moisture content in the cotton bale will also benefit the textile manufacturer. In this study, a standard carding atmosphere and a modified atmosphere of low temperature and high humidity were used as the treatments. Bales of the same cultivar and module were ginned sequentially in order to reduce the variability in the fiber properties. All cotton was processed on the same textile equipment. The only variable was the atmospheric conditions surrounding the card. The results of this work indicate that increasing the degree of saturation of the air surrounding the card by cooling the air and increasing the relative humidity minimizes the loss in moisture content of the cotton fiber through carding and reduces short fiber content in carded and finisher drawing sliver. Rotor yarn processing and quality were not affected by the treatment. Ring yarn processing efficiency, and ring and vortex yarn quality was improved in the cooler, moister environment sur­rounding the card.
Strang (1954) suggested that the air currents within the card affect the operation of the machine, and determined that the air surrounding the card was influenced by changes in vapor pressure, temperature, and humidity. Additionally, his work suggested that temperature (>10 °C) and relative humidity (50 to 55%) are important considerations for carding, but he did not discuss the effects of temperature and relative humidity on cotton fiber moisture content during carding. Sengupta et al. (1983) investigated the impact of various variables on carding forces (the force required to individualize fibers from tufts of fibers), and concluded that increased relative humidity resulted in decreased carding forces, which they attributed to the reduction of the flexural rigidity of the cotton fibers as a result of an increase in the moisture content of the fibers. The reduction in flexural rigidity of fibers as a result of increased moisture also reduced the breakage rate of fibers at carding (Sengupta et al., 1982). Increased relative humidity resulted in a reduced end breakage rate at spinning (Walker, 1964). In fact, McCreight et al. (1997) stated that the amount of water that fibers contain can greatly affect their physical properties. The absorption of moisture by cotton fibers changed the mechanical and frictional properties of the cotton, which affected the behavior of the fibers in processing (Morton and Hearle, 1997).

Although the research above cited increased relative humidity as a factor in improved carding, they did not indicate what the moisture content of the cotton is under the treatments investigated. In fact, there was no discussion in the scientific literature on temperature and relative humidity (RH) at the various processing stages of opening and carding of cotton fiber along with the moisture content of the fiber. It is reasonable to assume that the temperatures of certain components of a card, primarily the cylinder, will increase due to forces generated in overcoming friction, which in turn will increase the temperature of the local ambient, i.e. alter the microclimate. Since production areas in a mill are conditioned for temperature and humidity rather than for the micro-climate of each individual machine, a rise in temperature of the microclimate of the machine at a constant room RH would increase the drying capabil-
ity of the air. Brooker et al. (1975) cite an example of this in the grain drying process. If ambient air at 29.4 °C is heated to 37.8 °C and passed through the grain to be dried, the humidity ratio (grams of wa­ter/grams of dry air) of the air after passing through the grain is higher. The removal of moisture from the grain is cited as the reason for the increased humid­ity ratio of the air after passing through the grain. A better explanation of this concept is provided by Esmay (1974) through an explanation of the degree of saturation of air. Degree of saturation is defined as the ratio of the humidity ratio of moist air to the humidity ratio of saturated air at the same dry bulb temperature and vapor pressure; therefore, the higher the degree of saturation, the less moisture can be removed from a material as the air passes through it (Esmay, 1974). Following this logic, the standard atmosphere for a typical carding area in a mill (24.0 °C and 55% RH) would have a degree of satura­tion of 54.264%. In order to increase the degree of saturation, it is necessary to reduce the temperature and/or increase the relative humidity. The objective of this study was to determine the effects on cotton fiber moisture content and fiber and yarn quality as cotton is processed in a standard ambient environ­ment compared to an environment which minimizes the drying of the cotton fiber in processing.


MATERIALS AND METHODS
Eight bales of cotton were selected from one module that had been ginned sequentially on the same day. From these bales, 136.36 kg of fiber were taken from each bale for testing and spinning. Each 136-kg sample was split into two 68-kg lots, one for each of the two treatments. The treatments in the study were carding at ambient conditions (24.0 °C and 55% RH; designated AMBIENT), and card­ing in an environment that maximizes the degree of saturation based on the capability of the condition­ing system in the carding room. This treatment was designated COOL and was achieved by cooling the air to a temperature of 15.6 °C and raising the relative humidity to 75%. The cotton from each bale for each treatment was processed on the same equipment, including an opening and cleaning line consisting of blend hoppers (Fiber Controls; Gas­tonia, NC), an Axi-Flow (coarse cleaner), GBRA (mixer), RN (coarse cleaner), RST (fine opener), and DX (deduster) (all Truetzschler; Monchengla­dbach, Germany). Once through the cleaning line, the cotton was carded at 27.27 kg/hr (60 lbs/hr) on a Saco-Lowell card (Saco-Lowell; Easley, SC), which was located in a confined room in order to control the temperature and humidity surrounding the card. This older model card was chosen simply because it does not have the large volumes of air removed from around the cleaning point (as is common on modern carding), which would have prohibited the manipulation of the ambient air surrounding the card. The card sliver produced was 4,961 tex (70 grains/yd). Along the processing points in opening, cleaning, and carding, temperature readings of the ambient air surrounding the equipment, the air inside the equipment, and the connecting duct work used for transporting the cotton were taken every 10 min during the processing of each lot for each treatment. In addition, the temperature and humidity of the carding room was measured every 10 min during the processing of all lots, and the moisture content of the cotton samples for each lot per treatment was determined by the oven drying method (ASTM, 2001). Cotton samples were taken at the hoppers from the bale (before feeding), at the GBRA, at the RST, and at the coiler of the card.
After opening, cleaning, and carding, the resultant card sliver for each lot of each bale for each treatment was split three ways for processing into drawing sliver in preparation for spinning on ring, rotor, and vortex spinning systems. The rotor spinning sliver received one pass of drawing on an RSB draw frame (Rieter; Winterthur, Switzerland) with a leveler producing 4,961 tex (70 grain/yd) sliver and subsequently spun on a Schlafhorst SE-1 1 rotor spinning machine (Saurer Group; Charlotte, NC). Yarn was spun at 117,000 ro­tor rpm and a combing roll speed of 8,000 rpm with a G30 rotor and a twist multiple a of 115.14 producing a 29.53 tex (20/1 Ne) yarn.
Ring spinning sliver was processed through two passes of drawing; the first on an SB-951 (Rieter; Winterthur, Switzerland) (unleveled) and the second on the RSB draw frame (leveled) producing 4,252 and 4,961 tex sliver (60 and 70 grain/yd sliver), respectively. The finisher drawn sliver was then processed into roving on a Zinser 660 roving frame (Saurer Group; Charlotte, NC) producing a 787.4 tex (0.75 hank) roving at a flyer speed of 1200 rpm and a twist multiple a of 39.39. Yarn (29.53 tex (20/1 Ne)) was subsequently spun from the roving on a Zinser 321 ring spinner (Saurer Group; Charlotte, NC) at a spindle speed of 16,500 rpm and with a twist multiple a of 116.66.


clip_image002
Sliver for vortex spinning was processed through three passes of drawing, with the first two on the SB­951 (unleveled) and the third on the RSB (leveled) producing 4,606, 4,252, and 3,898 tex sliver (65, 60, and 55 grain/yd sliver), respectively. The finisher drawn sliver was then spun into 20/1 Ne yarn on a Muratec MVS 851 (Muratec; Charlotte, NC) vortex spinner at 350 meters/min.
All waste from opening, cleaning, carding, draw­ing, roving, and spinning was collected and weighed. Fiber length, uniformity, strength, micronaire, and color for each bale were measured on a High Volume Instrument (HVI) (Uster Technologies; Knoxville, TN). Test results for each treatment are shown in Table I. In addition, fiber length and short fiber con­tent were measured from in-process fiber and sliver on a Peyer AL-101 (Peyer; Knoxville, TN). Yarn processing efficiency was determined by recording the number of ends down during the processing of each lot for each treatment. In addition, yarn even­ness, regular occurring yarn faults (thick places, thin places, and neps), irregular yarn faults (major, minor, long thin places, long thick places), and yarn tensile strength were measured.
The design for this experiment was completely random with 8 bales, 2 temperature treatments, and 3 spinning systems resulting in a total of 48 spinning lots. Each lot was assigned a lot number (1 through 48) and the lots were run in random order by select­ing the lot order through a random number generator. All data were subjected to analysis of variance (SAS Institute; Cary, NC) to determine any significant effect of the treatments on the dependent variables (cotton moisture content, fiber properties, spinning efficiency, yarn properties). Significant differences between the means of the affected variables were determined by Duncan’s multiple range test (P = 0.05).
RESULTS AND DISCUSSION
Cotton fiber moisture content in the card sliver was affected by the environmental conditions in card­ing room (Table 2). The resultant sliver from the cool treatment retained most of its original moisture con­ tent in the bale, unlike the ambient treatment, which lost 0.5% of its original moisture content. The cool­ing effect of the cool treatment in the carding room did, in fact, reduce the temperature by approximately 7.5 °C under the card where the cylinder is located and over 9.0 °C at the doffer (Table 3). In addition,
clip_image004
the temperature of the sliver at the coiler was reduced by approximately 4.0 °C. It appears that the reduced drying capability of the cool environment resulted in little to no loss in the moisture content of the cotton through carding. In fact, the calculated degree of saturation of the cool versus ambient treatment is 74.66% and 53.98%, respectively. These values are based on actual average temperatures and relative humidity for each treatment of 15.81 °C and 75% RH for the cool treatment and 23.79 °C and 54.71% RH for the Ambient treatment. The degree of saturation numbers were calculated by the formula defined by Esmay (1974) as follows:
clip_image006
Fiber length was affected by the cool treatment in the form of reduced short fiber content (Table 4). There was a reduction of 1.69% at carding, 0.59% at ring spinning finisher drawing, 1.3% at rotor spinning finisher sliver, and 0.62% at vortex spinning finisher drawing. This result follows the conclusions by Sen­ gupta (1982) that the reduction in flexural rigidity of fibers, as a result of increased moisture, caused a reduction in the breakage rate of fibers at carding.
Yarn processing and quality for rotor spinning were not affected by the treatments, but ring spinning and vortex spinning were affected (Tables 5 and 6, respectively). The reason yarn processing and qual­ity for rotor spinning was not affected may lie in the fact that the fibers in the sliver fed to rotor spinning are combed and individualized by the combing roll, then drafted in a high-draft air stream through the fiber channel and reassembled in the rotor cup for yarn formation. It is widely known that rotor spinning tends to be more tolerant of short fiber content than ring and vortex spinning. Therefore, it is theorized that the improvement in the short fiber content of the sliver for the cool treatment for rotor spinning was not enough to override the favorable treatment of short fiber by this spinning system.
Ring and vortex spun yarn were affected in a similar manner by the cool treatment. Ring spin­ning in the cool environment improved spinning ef­ficiency and yarn evenness and reduced yarn faults. Vortex spinning in the cool environment improved
clip_image008
yarn evenness and a reduced yarn faults. It is widely known that short fibers affect spinning efficiency, yarn evenness, and yarn defects, especially in roller drafting systems like ring and vortex spinning. Un­like rotor spinning, the fibers in the sliver are not individualized and then reassembled for yarn forma­tion. A reduction in short fibers in slivers processed through a roller drafting system decreases the number of uncontrolled fibers in the drafting zone, which alters the mass evenness of the yarn and creates thick and thin places along the length of the yarn. In some cases, where the number of thin places is substantial, end breaks can occur. Yarn strength was not affected by the treatments, so it will not be discussed.
CONCLUSIONS
Reducing the drying capability of the air sur­rounding the card by increasing the degree of satura­tion of the surrounding ambient air (cool treatment) minimized the loss of moisture in the cotton fiber. As a result of minimizing the loss in moisture, short fiber content is reduced in card sliver and finisher drawing sliver regardless of the number of passes of drawing. This reduction in short fibers, as a result of the treat­ment, did not translate into improved rotor spinning performance or yarn quality. On the contrary, in the cool treatment yarn evenness was improved and yarn defects reduced for vortex and ring spinning, and efficiency was improved for ring spinning.
Read more...

Card Auto leveler

Analysis of the Work of a Card Autoleveller
with a New Algorithm of Operation
Abstract
These studies concern the work of a modernised autoleveller whose algorithm of operation allows for the phenomenon of sliver retardation after short-term regulation. The autolevel­ler’s effectiveness at standard and corrected controlling signals was compared. Measure­ments were made for cotton, viscose and polyester fibres, applying three different drafts in the autoleveller. It was demonstrated that the levelling capacity of the new autoleveller is much better than that of the traditional one.
Key words: autoleveller, card, evenness of mass.
Introduction
Long-term analyses of the operation of short-term regulation systems [2, 3] have shown that the regularity of the lin­ear density of slivers levelled by means of a short-term autoleveller is a function of time, and only its direct measuring in an on-line system enables immediate and reliable conclusions to be drawn about the effectiveness of the regulation proc­ess. The results of the studies conducted confirmed the need for a short-term autoleveller whose algorithm of opera­tion would allow for the phenomenon of sliver retardation. Analyses of sliver retardation phenomenon and of a typical algorithm of the operation of a short-term autoleveller led to changes in the autoleveller controlling system, aimed at achieving the minimum possible vari­ations in the linear density of sliver be­fore it is introduced to the next machine in the technological process. The new
algorithm of operation is presented in Equation (1)
clip_image002
where:
R ’(t) – the momentary draft in the au­toleveller with the correction of the controlling signal;
R(t) – the momentary draft in a classi­cal autoleveller;
a, b, c – coefficients of the equation of sliver retardation;
k – the limiting draft at which sliver
retardation does not occur.
Changes were made to a typical au­toleveller taking Equation (1) into ac­count. The new algorithm was realised digitally, on the basis of the correction system, in the form of a computer with relevant software. It was assumed that
only after retardation would the sliver reach the lowest value of irregularity of linear density, below CV = 2.7% acc. to Uster, at a linear density of about 4 ktex. At longer lengths, the values of CV coeff­icient should not exceed CV1m = 0.8%, CV3m = 0.5%.
Subject of analysis
The subject of our analysis was a modified short-term card autoleveller constructed as a separate test stand, independent of the card. It is presented in Figure 1.
Modification of the stand consisted in including a corrector of a controlling signal into the autoleveller controlling system. The main aim of this corrector is to change the autoleveller’s algorithm of operation.

clip_image004
clip_image006
Some of the more important constant parameters in these studies are:
the speed of the measuring feed roll­ers: Vz= 1.33 m/s (80 m/min);
the length of the drafting zone: 62 mm; n the measuring range of the inductive
linear displacement sensor: ± 0.7 mm;
the linear density of the feeding sliver:
6 ktex.
Variable parameters in the studies are:
raw material:
medium-fibre cotton (BS)
viscose fibres (WI)
polyester fibres - Elana (PE);
nominal drafts in the autoleveller:
1.2, 1.4, 1.6.
The program continuously corrects the value of a controlling voltage signal. It was written on the basis of the Delphi system by Borland. Figure 2 shows the main window of the programme where the user can set the parameters necessary to perform the regulation process cor-
rectly; in Figure 3 we see the regulation window with the correction of the con­trolling signal.
The programme works by continuously taking the voltage signal U(t) transmitted from the power amplifier to the drawing wobble-plate engine, and processing it in such a way so that the engine is supplied with voltage U’(t), that is, allowing for the sliver retardation phenomenon.
Results of analysis
27 variants of slivers were analysed. They were made of 3 raw materials at 3 different drafts in the autoleveller (1.2, 1.4, 1.6) Each sliver was made in the fol­lowing three ways: regulated according to the typical operation algorithm, regulated with correction of the controlling signal, and non-regulated. The slivers were tested three times on a Uster Tester 3: immediately (U 0), 1.5 hours (U 1.5) and 3.5 hours (U 3.5) after leaving the autoleveller; 81 measurements were made in total.
clip_image008


clip_image010
clip_image012
in the example diagrams in Figures 4 and 5.
R - regulation at correction of control­ling signal off;
K - regulation at correction of control­ling signal on.
The dependencies and tendencies ob­served in the changes of the analysed parameters of slivers showed very great congruity both for different raw materials and for different drafts in the autoleveller.
The autoleveller works much better with the modified operation algorithm. As early as 1.5 hours after the regulation process, the value of the coefficient of linear density variation CV acc. to Uster decreases (to a level lower than for the sliver regulated in a standard way) and the coefficient of levelling capacity in­creases. After 3.5 hours, the structure of regulated slivers stabilises after regula­tion (measurements made later did not show any significant changes in the ana­lysed parameters). The irregularity CV% of the slivers tested falls to the level of about 2.5-3.4%, that is, the values for all slivers are below the level recommended by Uster of CV=3.5%. By evaluating the levelling capacity of the autoleveller, we obtain values η above 30% (even up to obtain values η above 30% (even up to about 45%), which are within the range of satisfactory regulation. So far it has not been possible to obtain such high values during standard regulation, even when evaluation is made directly after regulation.
The nominal draft in the autoleveller
during regulation with correction of the controlling signal does influence the measurement results obtained. Draft R=1.4 turned out to be the best. With this draft, the lowest values of irregularity of linear density were obtained for all tested lengths. The levelling capacity of the au­toleveller was also the best.
Figure 6 shows some diagrams obtained from the analysis on the Uster Tester 3 apparatus for the best sliver variant.


Summary
Correcting the controlling signal during short-term regulation of draft consider­ably improved the regularity of the linear density of slivers with stabilised internal structure. If short-term regulation is per­formed correctly, it is possible to achieve the desired quality parameters of slivers.
The limit level CV=2.7% is a very re­strictive value. The Uster Company ac­cepts CV=3.5% as the maximum value for slivers of typical linear densities. If we follow Uster’s requirements, all the analysed slivers regulated with correc­tion of the controlling signal meet the qualitative criteria.
Although the autoleveller works on short lengths, good results of sliver irregularity were also obtained on longer lengths. It was possible to obtain the desired pa­rameters for several variants. In all other cases, the above-mentioned values were only slightly exceeded.
It was not possible to achieve the required level of irregularities of linear density of slivers levelled by a short-term autoleveller for polyester slivers, but the values CV=2.94%, CV1m=0.86% and CV3m= 0.60%, which were obtained for one of the variants, are very difficult to achieve in the case of the autoleveller’s standard work, that is, without any cor­rection of the controlling signal.
It was found that the best nominal draft in autoleveller was R=1.4 for cotton and viscose slivers, and R=1.2 for polyester slivers. Once more it was demonstrated that in order to obtain a low irregularity of regulated slivers, it is necessary to use small drafts in short-term autolevellers.
Read more...

CARDING

INTRODUCTION

"Card is the heart of the spinning mill" and "Well carded is half spun" are two proverbs of the experts. These proverbs inform the immense significance of carding in the spinning process.High production in carding to economise the process leads to reduction in yarn quality.Higher the production, the more sensitive becomes the carding operation and the greater danger of a negative influence on quality.The technological changes that has taken place in the process of carding is remarkable. Latest machines achieve the production rate of 60 - 100 kgs / hr, which used to be 5 - 10 kgs / hr, upto 1970.

THE PURPOSE OF CARDING:

  1. to open the flocks into individual fibres
  2. cleaning or elimination of impurities
  3. reduction of neps
  4. elimination of dust
  5. elimination of short fibres
  6. fibre blending
  7. fibre orientation or alignment
  8. sliver formation

TECHNOLOGICAL POINTS IN CARDING

  • There are two types of feeding to the cards
    1. feeding material in the form of scutcher lap
    2. flock feed system (flocks are transported pneumatically)
    • lapfeeding
      1. linear density of the lap is very good and it is easier to maintain(uniformity)
      2. the whole installation is very flexible
      3. deviations in card output will be nil, as laps can be rejected
      4. autolevellers are not required, hence investment cost and maintenace cost is less
      5. transportation of lap needs more manual efforts( more labour)
      6. lap run out is an additional source of fault, as it should be replaced by a new lap
      7. more good fibre loss during lap change
      8. more load on the taker-in, as laps are heavily compressed
    • flock feeding
      1. high performance in carding due to high degree of openness of feed web
      2. labour requirement is less due to no lap transportaion and lap change in cards
      3. flock feeding is the only solution for high prouduction cards
      4. linear density of the web fed to the card is not as good as lap
      5. installation is not felxible
      6. autoleveller is a must, hence investment cost and maintenance cost is more
    • Type of flock feed(chute feed)
      1. there are two basic concepts of flock feed
        1. one piece chute without an opening device
        2. two piece chute with an opening system
      2. one piece chute is simple, economical and requires little maintenance
      3. two piece chute is complex, expensive, but delivers a uniform batt.
      4. One piece chut is a closed system, i.e.excess flock returns to the distrbutor, if too much material is present, neps can be increased
      5. one piece chute is not flexible to run different mixings
      6. layout restrictions are more with one piece chute
    • A feeding device is a must to feed the web to the Taker-in region and it should perform the following tasks
      1. to clamp the batt securely throughout its width
      2. to grip the fibres tightly without slippage during the action of taker-in
      3. to present the fibres in such a manner that opening can be carried out gently
    • The divertor nose(sharp or round) and the length of the nose(guide surface) have a significant influence on quality and quantity of waste removed. Shart nose divertor avoids fibre slippage but the opening action is not gentle.
      If the length of the guide surface is too short, the fibres can escape the action of the taker-in. They are scraped off by the mote knives and are lost in the waste receiver.
    • Feed roller clothed with sawtooth is always better , because it gives good batt retention. Thus the opening effect of the taker-in is more as it is in combing
    • Rieter has devloped a "unidirectional feed system" where the two feed devices(feed roller and feed plate are oppositely arranged when compared with the conventional system. i.e. the cylinder is located below and the plate is pressed against the cylinder by spring force. Owing to the direction of feed roller, the fibre batt runs downwards without diversion directly into the teeth of the taker-in(licker-in) which results in gentle fibre treatment. This helps to reduce faults in the yarn.
    • The purpose of the taker-in is to pluck finely opened flocks out of the feed batt, to lead them over the dirt eliminating parts like mote knives, combing segment and waste plates, and then to deliver the fibres to the main cylinder. In high production cards the rotational speed ranges from 700-1400
    • The treatment for opening and cleaning imparted by Taker-in is very intensive, but unfortunately not very gentle.Remember that around 60% of the fibres fed to the main cylinder is in the form of individual fibres.
    • The circumferential speed of Taker-in is around 13 to 15 m/sec and the draft is more than 1000.It clearly shows that fibre gets deteriorated at this opening point. Only the degree of deterioration can be controlled by adjusting the following
      1. the thickness of the batt
      2. the degree of openness of the rawmaterial
      3. the degree of orientation of the fibres
      4. the aggressiveness of the clothing
      5. the distance between the devices
      6. the rotational velocity of the taker-in
      7. the material throughput
    • Latest TRUTZSCHLER cards work with three licker-ins compared to one liker-in.The first one is constructed as needle roll. This results in very gentle opening and an extremely long clothing life for this roll. The other two rollers are with finer clothing and higher speeds, which results in feeding more %of individual fibres and smallest tufts compared to single lickerin, to the main cylinder. This allows the maing cylinder to go high in speeds and reduce the load on cylinder and flat tops. There by higher productivity is achieved with good quality. But the performance may vary for different materials and different waste levels.
    • between the taker-in and main cylinder , the clothings are in the doffing disposition. It exerts an influence on the sliver quality and also on the improvement in fibres longitudinal orientation that occurs here. The effect depends on the draft between main cylinder and taker-in.The draft between main cylinder and taker-in should be slightly more than 2.0.
    • The opening effect is directly proportional to the number of wire points per fibre. At the Taker-in perhaps 0.3 points/ fibre and at the main cylinder 10-15 points /fibre.If a given quality of yarn is required, a corresponding degree of opening at the card is needed. To increase production in carding, the number of points per unit time must also be increased. this can be achieved by
      1. more points per unit area(finer clothing)
      2. higher roller and cylinder speeds
      3. more carding surface or carding position

      speeds and wire population has reached the maximum, further increase will result in design and technological problems. Hence the best way is to add carding surface (stationary flats). Carding plates can be applied at

      1. under the liker-in
      2. between the licker-in and flats
      3. between flats and doffer
    • Taker-in does not deliver 100% individual fibres to main cylinder. It delivers around 70% as small flocks to main cylinder. If carding segments are not used, the load on cylinder and flats will be very high and carding action also suffers. If carding segemets are used, they ensure further opening, thinning out and primarily, spreading out and improved distribution of the flocks over the total surface area.carding segments bring the following advantages
      1. improved dirt and dust elimination
      2. improved disentanglement of neps
      3. possibility of speed increase (production increase)
      4. preservation of the clothing
      5. possibility of using finer clothings on the flats and cylinder
      6. better yarn quality
      7. less damage to the clothing
      8. cleaner clothing
    • In an indepth analysis, all operating elements of the card were therefore checked in regard to their influence on carding intensity. It showed that the "CYLINDER-FLATS" area is by far the most effective region of the card for.
      1. opening of flocks to individual fibres
      2. elimination of remaining impurities(trash particles)
      3. elimination of short fibres( neps also removed with short fibres)
      4. untangling the neps
      5. dust removal
      6. high degree of longitudinal orientation of the fibres
    • The main work of the card, separation to individual fibres is done between the main cylinder and the flats Only by means of this fibre separation, it is possible to eliminate the fine dirt particles and dust.
      When a flat enters the working zone, it gets filled up very quickly. Once it gets filled, after few seconds, thereafter , hardly any further take-up of fibres occurs, only carding.Accordingly, if a fibre bundle does not find place at the first few flats, then it can be opened only with difficulty.It will be rolled between the working surfaces and usually leads to nep formation
    • In princile, the flats can be moved forwards or backwards, i.e. in the same direction as or in opposition to the cylinder.In reverse movement, the flats come into operative relationship with the cylinder clothing on the doffer side. At this stage, the flats are in a clean condition. They then move towards the taker-in and fill up during this movement.Part of their receiving capacity is thus lost, but sufficient remains for elimination of dirt, since this step takes place where the material first enters the flats. At this position, above the taker-in, the cylinder carries the material to be cleaned into the flats. The latter take up the dirt but do not transport it through the whole machine as in the forward movement system. Instead , the dirt is immediately removed from the machine. Rieter studies show clearly that the greater part of the dirt is hurled into the first flats directly above the taker-in.
    • Kaufmann indicates that 75% of all neps can be disentagled, and of these about 60% are in fact disentagled. Of the remaining 40% disentaglable nep
      1. 30-33% pas on with the sliver
      2. 5-6% are removed with the flat strips
      3. 2-4%are eliminated with the waste
      The intensity of nep separation depends on
      1. the sharpness of the clothing
      2. the space setting between the main cylinder and the flats
      3. tooth density of the clothing
      4. speed of the main cylinder
      5. speed of the flat tops
      6. direction of flats with reference to cylinder
      7. the profile of the cylinder wire
    • The arrangement of the clothing between the cylinder and the doffer is not meant for stripping action, It is for CARDING ACTION.This is the only way to obtain a condensing action and finally to form a web. It has both advantages and disadvantages.The advantage is that additional carding action is obtained here and it differs somewhat from processsing at the flats.A disadvantage is that leading hooks and trailing hooks are formed in the fibres , beause the fibres remain caught at one end of the main cylinder(leading hook) and some times on the doffer clothing(trailing hook).
    • There are two rules of carding
      1. The fibre must enter the carding machine, be efficiently carded and taken from it in as little time as possible.
      2. The fibre must be under control from entry to exit
    • Carding effect is taking place between cylinder and doffer because, either the main cylinder clothing rakes through the fibres caught in the doffer clothing, or the doffer clothing rakes thro the fibres on the main cylinder. Neps can still be disentangled here, or non-separated fibre bundles can be opened a bit in this area and can be separated during the next passage through the flats
    • A disadvantage of web-formation at the card is the formation of hooks. According to an investigation by morton and Yen in Manchester, it can be assumed that
      1. 50% of the fibres have trailing hooks
      2. 15% have leading hooks
      3. 15% have both ends hooked
      4. 20% without hooks
    • Leading hooks must be presented to the comber and trailing hooks to the ring spinning frame. There must be even number of passages between card and comber and odd number between the card and ringframe.

  • Read more...